PCB材料

PCB材料

370HR高速板材規格參數

       370HR層壓板是使用高性能180°C Tg FR-4多功能環氧樹脂制成的,該材料專為要求大散熱性能,可靠性和耐CAF性能的多層印刷線路板(高速PCB)應用而設計。 該材料具有出色的熱性能,且熱膨脹系數(CTE)低,并且其機械,化學和防潮性能達到或超過了傳統FR-4材料的性能,370HR用于數千種PCB設計中,并且在熱可靠性,CAF性能,易加工性和順序層壓設計的可靠性能方面被證明是同類產品中最好的。

 

 

PropertyTypical ValueUnitsTest Method
Metric (English)IPC-TM-650 (or as noted)
Glass Transition Temperature (Tg) by DSC180°C2.4.25C
Decomposition Temperature (Td) by TGA @ 5% weight loss340°C2.4.24.6
Time to Delaminate by TMA (Copper removed)

A. T260

B. T288

60

30

Minutes2.4.24.1
Z-Axis CTE

A. Pre-Tg

B. Post-Tg

C. 50 to 260°C, (Total Expansion)

45

230

2.8

ppm/°C

ppm/°C

%

2.4.24C
X/Y-Axis CTEPre-Tg13/14ppm/°C2.4.24C
Thermal Conductivity0.4W/mKASTM E1952
Thermal Stress 10 sec @ 288oC (550.4oF)

A. Unetched

B. Etched

PassPass Visual2.4.13.1
Dk, Permittivity

A. @ 100 MHz

B. @ 1 GHz

C. @ 2 GHz

D. @ 5 GHz

E. @ 10 GHz

4.24

4.17

4.04

3.92

3.92

2.5.5.3

2.5.5.9

Bereskin Stripline

Bereskin Stripline

Bereskin Stripline

Df, Loss Tangent

A. @ 100 MHz

B. @ 1 GHz

C. @ 2 GHz

D. @ 5 GHz

E. @ 10 GHz

0.0150

0.0161

0.0210

0.0250

0.0250

2.5.5.3

2.5.5.9

Bereskin Stripline

2.5.5.5

2.5.5.5

Volume Resistivity

A. After moisture resistance

B. At elevated temperature

3.0 x 108

7.0 x 108

MΩ-cm2.5.17.1
Surface Resistivity

A. After moisture resistance

B. At elevated temperature

3.0 x 106

2.0 x 108

2.5.17.1
Dielectric Breakdown>50kV2.5.6B
Arc Resistance115Seconds2.5.1B
Electric Strength (Laminate & laminated prepreg)54 (1350)kV/mm (V/mil)2.5.6.2A
Comparative Tracking Index (CTI)3 (175-249)Class (Volts)UL 746A
ASTM D3638
Peel Strength

A. Low profile copper foil and very low profile copper foil all copper foil >17 μm [0.669 mil]

B. Standard profile copper

    1. After thermal stress

    2. At 125oC (257oF)

    3. After process solutions


1.14 (6.5)


1.25 (7.0)

1.25 (7.0)

1.14 (6.5)

N/mm (lb/inch)

2.4.8C


2.4.8.2A

2.4.8.3

2.4.8.3

Flexural Strength

A. Length direction

B. Cross direction

90.0

77.0

ksi2.4.4B
Tensile Strength

A. Length direction

B. Cross direction

55.9

35.6

ksiASTM D3039
Young's Modulus

A. Length direction

B. Cross direction

3744

3178

ksiASTM D790-15e2
Poisson's Ratio

A. Length direction

B. Cross direction

0.177

0.171

ASTM D3039
Moisture Absorption0.15%2.6.2.1A
Flammability (Laminate & laminated prepreg)V-0RatingUL 94
Relative Thermal Index (RTI)130°CUL 796
The data, while believed to be accurate and based on analytical methods considered to be reliable, is for information purposes only. Any sales of these products will be governed by 

 